MIX DESIGNS

 

ROOF FILLS

MIX DESIGNS
Cement to Perlite Ratio (by vol.) Cement (Kgs) Perlite Construct (m³) Water (Liters)
¼ 375 1 300
300 1 290
250 1 270
190 1 270
TECHNICAL PROPERTIES
Wet Density (Kg/m³) Dry Density (Kg/m³) Compressive Strength (MPa) Thermal Conductivity (W/mK)
808 640 3,45 0,10
728 544 2,35 0,09
648 448 1,38 0,08
584 384 0,86 0,07

 

 

FLOOR SCREEDS

MIX DESIGNS
Cement to Aggregate Ratio (by vol.) Cement (Kgs) Perlite Construct (m³) 0-5 mm SAND (m³) Water (m³
¼ 350 0,5 0,5 0,3
300 0,5 0,5 0,3
250 0,5 0,5 0,3
¼ 350 0,75 0,25 0,27
300 0,75 0,25 0,27
250 0,75 0,25 0,27
TECHNICAL PROPERTIES
Wet Density (Kg/m³) Dry Density (Kg/m³) Compressive Strength (MPa)
1800 1700 20-25
1700 1600 15-20
1600 1500 12-15
1300 1200 8-12
1200 1100 7-10
1100 1000 5-8

 

 

 

Impartial laboratory test data of Robert W. Hunt Co. Engrs under sponsorship of the Perlite Institute INC. Strength data based on ASTM Type I Portland Cement. Neutralized vinsol resin or other air entrainment agent is used in all mix designs, according to manufacturer's recommendations. Exact quantity of water depends on site conditions and can be adjusted to achieve the required density. The 1:6 mix ratios is the standard mix used on most roof deck applications.